高级检索

    铜冶炼颗粒汞砷铊形态分布与浸出风险研究

    Speciation Distribution and Leaching Risks of Mercury, Arsenic and Thallium in Copper Smelting Particles

    • 摘要: 铜冶炼颗粒含汞、砷、铊等有毒元素,但其形态分布与浸出风险尚不明确,尤其缺少对细颗粒的研究。本文以云南某铜冶炼厂经静电除尘器收集的颗粒为对象,研究总颗粒和细颗粒(<25 μm)中汞、砷、铊等有毒元素的形态分布特征与浸出风险。采用X射线衍射分析(XRD)、扫描电子显微镜−能谱分析(SEM-EDS)、X射线荧光光谱(XRF)、X射线光电子能谱(XPS)、电感耦合等离子体质谱(ICP-MS)等多尺度表征方法,并结合酸溶态/残渣态两步提取、程序升温分解和浸出实验,揭示汞、砷、铊的赋存形态及浸出行为。结果表明,Hg以难溶性HgS形态存在,细颗粒中可能含少量HgSO4。总颗粒中As呈表面富集特征,细颗粒中As在体相与表面分布趋于均匀,以As3+和As5+混合价态共存,细颗粒中As3+占比由18.8%增加至41.0%,说明细颗粒中As更多以As2O3或亚砷酸盐存在。Tl在总颗粒和细颗粒中总含量分别约29.0 g/t和4.1 g/t,酸溶态分别占96.9%和94.7%,推测以高溶解性Tl化合物为主。浸出实验在固液比1∶100、70 ℃、200 r/min条件下进行1 h。结果表明,Tl浸出风险最高,总颗粒在5% H2SO4中Tl浸出率达86.5%,细颗粒在10% H2SO4和15% H2SO4中Tl浸出均超过90.0%,细颗粒Tl浸出风险高于总颗粒。Hg浸出率较低,但酸性条件下存在不可忽视的溶出风险。As浸出率虽低于10%,但总量较高,且细颗粒中毒性As3+占比更大,其长期环境行为仍需重视。本研究为铜冶炼颗粒的解毒提供了参考,Tl可通过水洗/稀酸浸出脱除,Hg主要以HgS形式存在,需经高温焙烧去除,As则需通过氧化As3+为As5+实现解毒。

       

      Abstract: Background Copper smelting electrostatic precipitator particles contain toxic elements such as Hg, As, and Tl, but their speciation distribution and leaching risks remain unclear, particularly regarding fine particles. This study investigated the distribution characteristics and leaching risks of these highly toxic elements—namely mercury, arsenic, and thallium—in both total particulate matter and fine particulate matter (< 25 µm) collected from an electrostatic dust precipitator at a copper smelting plant in Yunnan, China. Methods Using multi-scale characterization techniques including XRD, SEM-EDS, XRF, XPS, and ICP-MS, combined with sequential extraction for acid-soluble fractions, temperature-programmed decomposition, and leaching tests, we revealed the occurrence forms and leaching behaviors of mercury, arsenic, and thallium. Results The results showed that As in the total particulate matter exhibited surface enrichment characteristics, whereas As in the fine particulate matter was distributed uniformly between the bulk phase and the surface. As existed in a mixed valence state of As3+ and As5+, and the proportion of As3+ in fine particles increased from 18.8% to 41.0%, indicating that As in the fine particulate matter was more likely to exist as As2O3 or arsenites. The total contents of Tl in the total and fine particulate matter were approximately 29.0 g/t and 4.1 g/t, respectively, with acid-soluble fractions accounting for 96.9% and 94.7%, respectively, and the dominant species being highly soluble Tl compounds. Hg existed primarily as insoluble HgS, while a small amount was potentially present as HgSO4 in the fine particulate matter. Leaching experiments were conducted at a solid-to-liquid ratio of 1:100, 70 °C, and 200 rpm for 1 h. The leaching tests showed that the release risk of Tl was the highest, with an extraction rate of 86.5% in 5% H2SO4 for the total particulate matter. The leaching rates of Tl from fine particulate matter in 10% and 15% H2SO4 exceeded 90.0%, indicating that the leaching risk of Tl in the fine particulate matter was higher than that in the total particulate matter. Although the leaching rate of Hg was relatively low, its leaching risk under acidic conditions remained non-negligible. Furthermore, while the leaching rate of As was lower than 10%, its total content was relatively high, and the higher proportion of toxic As3+ in fine particulate matter suggested that the long-term environmental behavior of As warranted close attention. Conclusions This study provides a reference for the detoxification of copper smelting particles. Tl can be removed by water washing or dilute acid leaching; Hg mainly exists as HgS and requires high-temperature roasting for removal, whereas As requires detoxification via oxidation from As3+ to As5+.

       

    /

    返回文章
    返回